Hi Gang,
I am laminating two flat poleyester based fiberglass pieces together. They are about 2 1/2 wide x 30" long. What is the best adhesive - Polyester resin, Epoxy resin, 5200 or ____?
Thanks,
Jim T.

 
    
AuthorReply
Jim Thompson

No ideas ??

March 24 2009, 5:05 PM 

I have only had one email with an opinion. I thought you guys would have some more ideas.
Thanks,
Jim T.

 
 
Phil J Mitchell

Adhesive

March 24 2009, 5:17 PM 

I'd rough them with 80g sandpaper, clean them with alcohol and use an epoxy. You might want to thicken it some.

West Systems has some great information on repairing polyester layups with epoxy. You can call their tech line.


Phil

 
 
Greg Isaac

Re: Adhesive

March 24 2009, 6:32 PM 

Epoxy and a layer of matting to make up the voids would work very well. You could get trick and vacuum bag it for the ultimate job....

 
 
Phil J Mitchell

Matting vs cloth

March 24 2009, 7:46 PM 

I read in the WEST SYSTEMS documentation that matting is coated with a material that dissolves when exposed to polyester resins. Since epoxy does not have this chemical in it, matting can be hard to use with epoxy. I've always used glass cloth with epoxy as a result of reading this. I figure the West guys know more about epoxy than I do. And that's not saying much.....

I like the bag idea though. you can really control the resin saturation when you use a bag and some vacuum.


Phil

 
 
Jim Thompson

Read the same thing

March 24 2009, 8:10 PM 

I have read the same thing but have not done any testing, and after hearing this again, I will probably not do and testing.
Jim T.

 
 
Greg Isaac

Read again.....

March 24 2009, 8:27 PM 


 
 
Phil J Mitchell

Chopped Strand Mat

March 25 2009, 8:43 AM 

Greg,

Good information. Yet I also read in that there are some issues still depending on where the mat was made and how.

I've never tried the stitched mat so that might be an option.


 
 
Greg Isaac

Re: Chopped Strand Mat

March 25 2009, 9:11 AM 

Ok, I surrender. I will do my thing my way, it has worked for me on the parts I have made that's all I can say. Good luck with your project.....

 
 
john nebelecky

Re: Adhesive

March 25 2009, 8:01 PM 

West System thickened with Cabosil. Scuff both surfaces with 36 grit, bag it if you have the means.
John

 
 
Jim Thompson

5200

March 26 2009, 8:09 AM 

Is there anyone that likes 5200 ???

 
 
John Harvey

5200

March 26 2009, 9:10 AM 

Jim, a friend and master boat builder once told me never glue anything together with 5200 you want to ever take apart. 5200 is a air dry compound that I have had a bad experience with installing windows in my sailboat as it did not cure.

West Epoxy is hard to beat, no matter what application. I have re-glued 200 year old furniture with the best results.

If you go 5200, they now have a fast cure product.

JH

 
 

Chris Hall, Jr.

5200

March 26 2009, 9:35 AM 

We used to use 5200 when mounting outboard motors. A 225 hp motor, yes 225, will hang on the transom of a boat with 5200 with no bolts installed when cured. You literally have to destroy fiberglass to get it free.

 
 
Dave Richardson

5200

March 26 2009, 9:39 AM 

3M5200 is a wonderful product in both above and below water applications where you want a tenasious bond plus and importantly the ability to flex and give a bit as the skins move. I too am an avid sailor and use 5200 for hull to deck joints, thru-hulls etc. Wooden boat restoration shops use it extensively with many differences of opinion in bonding the planking or skin to battens and frames. The advantage of this over epoxy is evident in its ability to give as the structure flexs. Epoxy does not give and as Morgan Marine found out, much to their chagrin when epoxy does flex it cracks allowing moisture ingress into the wood that is being bonded. The obvious detraction however is if you want to remove something that has been put together with 5200 the only way I know is to run a router through it. Of course epoxy isn't exactly easy either. The original long cure version 5200 works well for a couple of hours and cures in a week. The short cure 4200 is workable for a far shorter period and when cured does not have the same tenacity as 5200. Bottom line is there is a home for 5200 and a much larger useage field for epoxy. 5200 or 4200 have a very short shelf life. Check the date codes on the tube carefully. MOST of what our West Marine carries is already out of date and either won't cure or won't come out of the tube. The date code on the tube is a use before code.

The other warning on 5200 - a single drop that goes where you don't want it will be tracked over everything you step on and be there forever. The teak deck on my sailboat knows this too well.

If you want to read about 5200 use from it's prime advocate in wooden boat restoration pick up Don Danenburg's 2 books.

 
 
phil spruit

gluing

March 26 2009, 9:41 AM 

Jim,
You never really specified what these parts are going to do, how square/even the 2 mating surfaces are, and how thick the 2 fiberglass parts are.
I would tend to think all glues mention would work, to a point. Heck, I got some double faced tape here at the shop that could bond those 2 together.

 
 
Greg Isaac

Re: 5200

March 26 2009, 9:47 AM 

I use 5200 to mount my rudder and turn fin brackets. As noted upon removal it will rip the plywood apart. A trick for that is heat. If I need to remove my brackets a propane torch used carefully will get it to let go. Then you have one heck of a mess. I'd rather deal with th removal issues that have a rudder or fin come off at 100+mph. Been there done that, NOT FUN!!!!!

 
 

Michael Hill

Danenburg has great forum too...

March 26 2009, 11:34 AM 

This is my understanding of 5200 too, Dave. Both of Don's books are great resources and he also has a great free forum on his website with lots of good info:

http://www.danenbergboatworks.com/

Michael

 
 
Dave Richardson

More 5200

March 26 2009, 12:28 PM 

If any of you are interested the link for 3M5200 Tech Specs is

http://multimedia.3m.com/mws/mediawebserver?66666UuZjcFSLXTtlx&EO8TVEVuQEcuZgVs6EVs6E666666--

A couple of other items;

5200 is not hardened by exposure to air. It is the moisture in the air that cures it. At 90% RH 70 degrees F it goes off in about 3 hours. Much longer with lower RH.

3M does not recommend it for installation of glass. Sika makes a product for glass that I have used on my sailboat.

Cleaning with alcohol prior to using it will prevent it curing.

There is a great table in the spec showing shear strength with various materials. As Craig mentioned the wood will tear off before this stuff shears.


 
 
John Harvey

More 5200

March 26 2009, 1:49 PM 

I wasn't using it on glass, rather acrylic or lexan. It does make a mess. As for the alcohol, that is possible. I once owned a "Rampage Yachts" center console, that had teak trim on the top of the console. I removed it to re-finish, and removed the jelcoat as well as a layer of glass came with the teak. 5200 the culpret and the teak had to be replaced...

A friend, James Jones, has built a new "vintage" hydro, out of more conventional materials than most builders, and assembled the entire boat with 5200. He litterally lives "Down East" in North Carolina, I beleive Larry made him a set of cowlings, the hull is a Glen L design I beleive. He has a 327 corvette engine installed, direct drive, flange from shaft bolted to engine, as well no thrust bearing.

I guess he can verify that 5200 is the best glue/sealer. Hopefully he will bring the boat out this summer.

 
 
Tommy Peters

5200

March 26 2009, 2:09 PM 

I once saw Derick Guthrie at Guthrie Boat Works in Wanchese, NC take West System, Clear Coat, several other epoxies, 5200, and outdoor carpenters glue, and clamped juniper sticks to a boat bottom and let them cure to see what glue was the strongest. They took a scale and pulled on the stick to see what the point was where the joint failed. 5200 was by far the strongest. And it flexes. Someone told me once that if you want it to kick off to touch the end of the joint with water after you glue something. It will even kick off under water. Have also heard of people knocking holes in a boat and patching the bottom with plywood, nails and 5200 to get home. It kicked off and they had a hard time removing the patch after they got her pulled up.

I use WD 40 to clean up after using it. Spray it on and wipe it off.

Something else that is cool is vinegar and West System (all epoxies). You can get glue all over your hands, pour some vinegar on it and rub the vinegar all over your hands. Then wipe it off. Unlike acitone, laquer thinner or other things I have tried it completly gets the glue to come off. Just wipe it off with a rag. No explosive, caustic chemicals.

 
 
 